Ingxubevange
Ingxubevange yobushushu obuphezulu
◆ I-alloy20cb-3 inokumelana okuhle kakhulu noxinzelelo lwe-corrosion cracking kunye nokuchasana okulungileyo kwindawo yokunciphisa i-corrosion ye-compound medium, kwaye isetyenziswe kwindawo ye-sulfuric acid kunye nofakelo lwemizi-mveliso yesisombululo se-sulfuric acid equkethe i-halogen ions kunye ne-ion zetsimbi.
◆ I-alloy28 isetyenziswa ngokubanzi kwi-papermaking, i-pharmaceutical, ikhemikhali, ukukhuselwa kwendalo, ukwakhiwa kweenqanawa kunye namanye amashishini.
◆ I-alloy31 (N08031 / 1.4562) yi-nitrogen ene-iron-nickel-molybdenum alloy esebenza phakathi kwe-super austenitic stainless steel kunye ne-alloys ekhoyo ye-nickel-based.Ifanelekile kwiikhemikhali kunye ne-petrochemical, ubunjineli bokusingqongileyo kunye neoli kunye negesi yemveliso, njl njl.
◆ I-Alloy33 luhlobo lwezixhobo zetsimbi ezisebenza ixesha elide phantsi kobushushu obuphezulu be-600-1200 ℃ kunye noxinzelelo oluthile.Inamandla aphezulu obushushu obuphezulu, i-anti-oxidation elungileyo kunye nokusebenza kwe-anti-corrosion.
◆I-Alloy75 inozinzo oluhle lwezicubu kunye nokuthembeka kwenkonzo phantsi kweemeko eziphezulu zokushisa, kwaye ifanelekile kwi-aerospace, i-aviation, i-petroleum, imboni yeekhemikhali, kunye nezinto ezibalulekileyo kwiinqanawa.
Ukwakhiwa kweekhemikhali
IBanga | C | Si | Mn | S | P | Cr | Ni | Fe | Al | Ti | Cu | Mo | Nb | enye |
akukho mkhulu kune | ||||||||||||||
Inconel600 | 0.15 | 0.5 | 1 | 0.015 | 0.03 | 14 ~ 17 | isiseko | 6~10 | - | - | ≤0.5 | - | - | - |
Inconel601 | 0.1 | 0.5 | 1 | 0.015 | 0.03 | 21-25 | isiseko | 10~15 | 1 - 1.7 | - | ≤1 | - | - | - |
Inconel625 | 0.1 | 0.5 | 0.5 | 0.015 | 0.015 | 20 ~ 23 | isiseko | ≤5 | ≤0.4 | ≤0.4 | - | 8~10 | 3.15–4.15 | Co≤1 |
Inconel725 | 0.03 | 0.2 | 0.35 | 0.01 | 0.015 | 19 ukuya ku-22.5 | 55 ~ 59 | Hlala | 0.35 | 1 - 1.7 | - | 7 ~ 9.5 | 2.75~4 | - |
Inconel690 | 0.05 | 0.5 | 0.5 | 0.015 | 0.03 | 27-31 | ≥58 | 7 ~11 | - | - | ≤0.5 | - | - | - |
Ubuncinci bepropathi ye-alloy
IBanga | urhulumente | amandla okuqina RmN/m㎡ | Amandla eSivuno Rp0.2N/m㎡ | Elongation As% | Brinell ubulukhuni HB |
Ingxubevange20cb-3 | Unyango lwesisombululo | 600 | 320 | 35 | - |
Ingxubevange28 | Unyango lwesisombululo | 680 | 347 | 37 | - |
Ingxubevange31 | Unyango lwesisombululo | 650 | 350 | 35 | 25 |
Ingxubevange33 | Unyango lwesisombululo | 770 | 320 | 34 | - |
Ingxubevange75 | Unyango lwesisombululo | 750 | 310 | 37 | - |